Development of wound healing scaffold using ZnO and TiO2 nanoparticles | Research Square window.SnipcartSettings = { analytics: { enabled: false } }; (function() { var accessVector = localStorage.getItem('access_vector') || ''; window.dataLayer = window.dataLayer || []; if (accessVector) { window.dataLayer.push({ user: { profile: { profileInfo: { snid: accessVector } } } }); } })(); (function(w,d,s,l,i){w[l]=w[l]||[];w[l].push({'gtm.start':new Date().getTime(),event:'gtm.js'});var f=d.getElementsByTagName(s)[0],j=d.createElement(s),dl=l!='dataLayer'?'&l='+l:'';j.async=true;j.src='https://www.googletagmanager.com/gtm.js?id='+i+dl;f.parentNode.insertBefore(j,f);})(window,document,'script','dataLayer','GTM-K279D39R'); Browse Preprints In Review Journals COVID-19 Preprints AJE Video Bytes Research Tools Research Promotion AJE Professional Editing AJE Rubriq About Preprint Platform In Review Editorial Policies Our Team Advisory Board Help Center Sign In Submit a Preprint Cite Share Download PDF Research Article Development of wound healing scaffold using ZnO and TiO2 nanoparticles Fatemeh Samadian, Younes Beygi-Khosrowshahi This is a preprint; it has not been peer reviewed by a journal. https://doi.org/ 10.21203/rs.3.rs-3833998/v1 This work is licensed under a CC BY 4.0 License Status: Posted Version 1 posted You are reading this latest preprint version Abstract The goal of this experiment is to produce a nanocomposite porous scaffold, using an electrospinning method that has biological properties to use as a skin tissue engineering (TE) and wound dressing. Polyhydroxyethyle methacrylate (PHEMA), polycaprolactone (PCL), Titanium oxide (TiO 2 ) nanoparticles, and zinc oxide (ZnO) nanoparticles, used to fabricate this scaffold. After the polymers were synthesized, both polymers were dissolved in chloroform, and nanoparticles were added. The diameter of the fibers obtained depends on the amount of addition of each nanoparticle, the injection rate of the device and the voltage, and the distance between the collector and the needle. Scanning electron microscopy (SEM) images showed the morphology of the scaffold and the cells can adhere well to nanofibers. The mechanical property test showed appropriate mechanical properties for this polymeric scaffold. X-ray diffraction pattern (XRD) and Fourier transform infrared spectroscopy (FTIR) results confirm the successful loading of nanoparticles into the polymer scaffold. Other biological features are characterized with, in vivo assay and MTT and antibacterial assay. The results show that this scaffold is suitable to use as a skin tissue scaffold and wound dress. electrospinning scaffold wound Zinc oxide Titanium oxide Figures Figure 1 Figure 2 Figure 3 Figure 4 Figure 5 Figure 6 Figure 7 Figure 8 Figure 9 Figure 10 1. INTRODUCTION The skin is the body's most important barrier against microorganisms and harmful substances. This barrier works best when healthy. Skin wounds can become infected and bacteria on the surface of the skin enter the body's bloodstream. Nowadays tissue engineering products promising for the treatment of skin lesions such as wounds and deep burns. Tissue engineering tries to restore the biological activities of damaged tissue to its original state by creating artificial tissue, and therefore plays a key role in wound healing and tissue replacement Interactions between biomaterials and tissues are highly dependent on the external surface structure of these substitutes. In this regard, the selection of the appropriate scaffold and cell plays a decisive role in achieving skin tissues that have similar characteristics in terms of histology and physiology to normal skin. Tissue engineering employs engineering and biological science principles and methods for the production and development of biological alternative Scaffolds, cells, growth factors and the main components of tissue engineering include polymers. The scaffold is a three-dimensional structure that is used as a framework to guide cells and it is a replacement for the extracellular matrix [ 1 ]. The structure of the scaffold must be possible for cells to adhere to it and it should be porous so when implanted on the body, the veins penetrate the scaffold and can feed the cells. One of the main characteristics of scaffolding is its degradability. The scaffold is gradually destroyed after the tissue is formed. Polymers are usually the best materials for tissue scaffolds than ceramics because polymers have better plasticity. Among different polymers, polycaprolactone has excellent mechanical properties including good biodegradability, low anti-genius, simple processability, non-toxic products resulting from its destruction. [30] Biodegradable electrospun PCL nanofibers, due to their advantages such as high surface to volume ratio in comparison with traditional scaffolds, are increasingly used for tissue engineering. Another material that is used in this article is poly hydroxyethyl methacrylate that is a nontoxic sterile polymer composed of 2-hydroxy ethyl methacrylate monomeric units. HEMA has a hydrophobic structure and hydrophilic cells are unable to adhere to the polymer surface. The cells are non-stick and suspended in 3D space between the environment and the polymer [ 2 ]. pHEMA has high solubility in organic solvents such as methanol and ethanol [ 3 ]. Furthermore, good mechanical stability, high biocompatibility, and physiological properties make pHEMA very useful used in biomedicine. Recently, nanomaterials have been widely used in many fields due to the development and growth of nanotechnology. Zinc oxide and titanium oxide nanoparticles due to their anti-cancer, anti-bacterial, anti-inflammatory, and binding properties, are used in many fields like drug delivery, food additives, and tissue engineering. Zinc oxide has received much attention due to its unique surface and chemical properties and various functions in ultraviolet emitters, chemical sensors and piezoelectric devices, etc. Moreover, Titanium oxide, due to its special properties, has an amazing ability to destroy the walls of prokaryotes, such as Escherichia coli [ 4 , 5 ]. In recent years, electrospinning with the ability to create polymeric nanofibers similar to the extracellular fibrous structure has attracted a lot of attraction. Electrospun nanofibers have many different applications in the fields of tissue engineering [ 6 , 7 ], energy storage [ 8 ], filtration [ 9 ], drug release[ 10 ], etc [ 11 ]. Combining nanoparticles and adding them to a polymer solution and electrospinning this solution and obtaining nanofibers containing nanoparticles is an up-to-date and interesting research field [ 12 ]. The diameter of the fibers obtained from the electrospinning process may vary from ten nanometers to several micrometers. Polymeric or composite solutions and high voltage sources are used to prepare electrospun nanofibers [ 13 , 14 ]. One of the advantages of producing nanofibers by electrospin method is that the direction and size of the fibers can be controlled and also the rate and speed of fiber production can be controlled [ 15 ]. Simulation of the extracellular matrix fibrous arrangement in the body, high surface to volume ratio, and significant porosity are the most important benefits of electrospinning. Parameters such as polymer molecular weight, concentration, surface tension, viscosity and conductivity of polymer solution, voltage, injection rate, spinner and collector type, and environmental conditions control the electrospinning process [ 16 ]. In this research, by using the conventional and inexpensive electrospinning method with using biodegradable and biocompatible polymers like polycaprolactone (PCL) and polyhydroxy ethyl methacrylate (pHEMA) and ceramic nanoparticles such as TiO 2 and ZnO, we tried to investigate the effect of the composite of these materials on the recovery time and absence of germs and infection at the wound site. 2. Method and Materials These materials have used in this experiment: TiO2(Mw = 79.866) and ZnO(Mw = 81.40) nanoparticles, pcl(Mw = 80 kDa), pHEMA(Mw=-kDa), phosphate buffer saline(PBS, ph = 7.4), Roswell Park Memorial Institute Medium(RPMI medium), Fetal Bovine Serum(FBS, Gibco company), 3(4,5dimethylthiazol-2yl)-2,5diphenyltetrazolium bromide(MTT), Ketamine, 70% ethanol solution 2.1 Polymer Synthesis The p-H was synthesized by CL, HEMA, and nanoparticles (TiO2 and ZnO). First, Sn(Oct)2 (30 mg, 0.074 mmol( was mixed with HEMA (3.8 g, 0.029 mol) in a round-bottom flask at room temperature until Sn(Oct)2 is completely dissolved. Then, CL (10 g, 0.0877 mol) was heated up to 130°C in a stirred round-bottom flask. The HEMA/Sn(Oct)2 solution was then added to the flask, and the reaction was carried out for 2 h. The synthesis and nanoparticle loading procedure was shown in figure (1). Figure 1 2.2 Fiber Preparation The precursor solutions for electrospinning were prepared in a two-stage approach. First, a suspension of inorganic powder in the solvent mixture was achieved by dispersing 0.5 g of solid in 10 mL of chloroform, all being ultrasonicated for 5 min at 50% amplitude. Then, 1.6 g of polymer was dissolved in the previously prepared suspension, which led to a final solution with 16% PCL and 5% inorganic powder; this was maintained under magnetic stirring for 24 h for PCL solubilization and general homogenization. 2.3 Electrospinning process The obtained solution was injected into a 5ml plastic syringe with a metallic needle and subjected to the electrospinning process. In this process electrical field was 19kv, the feeding rate was 0.5 ml/h and the distance from needle to collector was 18 cm. 2.4 SEM characterization To determine the characteristics of electrospun scaffolds, scanning electron microscopy (SEM) has used. To increase electrical conductivity, the surface of the scaffold was first covered with a thin coating with a thin layer of gold. The device used in this test is manufactured by Philips Netherlands and the model of the microscope is XL30. 2.5 XRD Characterization Another analysis used to study the Phase composition and crystallization of scaffolding is X-Ray ((XRD) Philips TW 3710) diffraction. X-ray diffraction analysis (XRD) has been used to investigate the composition of atoms in the structure of polymer crystals. After reviewing the results obtained from X-ray diffraction analysis, it can be seen that the nanoparticles are loaded into the structure of polymer fibers. 2.6 FTIR Characterization To comment on the loading of nanoparticles into polymer fibers and their reaction with polymer functional groups and to identify the functional groups present in the sample, a device Nicolet nexus 670 at a wavelength of 400-30000 cm − 1 has been used. 2.7 Contact Angle test Goniometer model CA-500A is used to measure the wettability of polymer nanofibers and the contact angle measurement model was sessile drop method. Distilled water is carefully poured on dry samples and in different cases, the contact angle is measured and photographed. The measurement is repeated several times for greater reliability and the contact angle is recorded when the error of the two data is less than 5%. 2.8 mechanical properties In addition to factors such as biocompatibility and porosity and biodegradability, mechanical properties are also the main features of a suitable scaffold. For this test, a 3*8 cm sample was used. Tension and strain testing device Z 010, Zwick/Roell, Ulm, Germany, has been used. 2.9 Bio-Degradability assay To evaluate the stability of polymeric scaffolds and measuring the rate of destruction in the body environment, hydrolytic and enzymatic biodegradability test was used. Therefore, the scaffolds were weighed (dry weight) and placed in a phosphate-buffered saline solution (PBS) containing 4 mg/ml trypsin enzyme for one month. During 15 days of biodegradability testing, each week the scaffolds were dried in a freeze dryer and their dry weight was measured. It should be noted that the scaffolding medium was changed weekly and by the end of the fourth week, the remaining mass percentage of the scaffolds was obtained from the following equation. The test was repeated three times for each sample to obtain the mean and standard deviation. Weight lost (%) = \(\frac{Wi-Wf}{Wi}\times\) 100 W i is the weight of nanoparticle loaded scaffold in dry state and W f is the final wet weight. 3. Biocompatibility analysis 3.1 Cell culture Skin fibroblast cells were cultured in a tissue culture flask and containing RPMI (cell culture media),1% antibiotic, and 10% FBS (fetal bovine serum), then incubated at 37°C, 5% CO2 and 90% humidity. During this experiment, cell culture media was changed every 2 days. 3.2 Cell viability assay This experiment is conducted in both direct and indirect ways. For analysis of proliferation and viability of cells, 4×10 4 cells (mouse fibroblast cells, CRL-2017) were seeded in 24 well plates in the presence of sterilized fibrous scaffold, and then RPMI media was added and 48 hours stayed at CO2 incubator under 90% air condition and 5% CO2 at 37 C. After 48 h, the MTT solution was added into each well and kept in dark condition inside of the CO2 incubator. After spending 8 h, DMSO was added to dissolve formazan crystals. UV spectrometer at a wavelength of 570 nm was used to measure absorbance. 3.3 Cell adhesion assay For measuring cell attachment, scaffolds (sterilized scaffold) were put into 6 well plates then 4×10 4 cells per well and media was added in each well. The sample was incubated for 8 hours and then the media was changed with new RPMI media. In this step, the sample was washed with PBS solution and glutaraldehyde was used as a fixator. After that fixator was removed, samples were washed with deionized water. The attached cells were observed with electron scanning microscopy (SEM). There may be three modes in the interaction between the cell and the polymer scaffold [ 17 , 18 ]. In the first type, the interaction between the cell and the polymer scaffold is non-adhesive, in other words, no interaction occurs and in the second type, the cells interact with each other but can easily separate. This type of adhesion is called inactive adhesion. In the second type, the surface response is controlled by physicochemical interactions between the polymer surface, adsorbed proteins, and adhesive cells [ 19 , 20 ]. In the third type, the cells interact spontaneously and strongly and adhere firmly to the surface of the polymer. 3.4 Antibacterial properties As mentioned earlier, TiO2 and ZnO nanoparticles have antibacterial properties that can be examined using gram-negative and gram-positive bacteria due to agar diffusion. For this test Escherichia coli (E. coli) from the Enterobacteriaceae family as gram-negative bacteria and Staphylococcus aureus from Staphylococcaceae family as gram-positive bacteria are used. The diameter of the circular scaffolds is one centimeter and we test the scaffolds with 2.5% and a scaffold without nanoparticles. Nutrient agar media was poured into a bacterial culture plate and after that media dried, bacteria cultured on this. Then we place the samples on the plate and after that plate was kept in an incubator at 37 C for 24 h. Lack of bacterial growth around the samples is evident that has shown in pictures. 3.5 In vivo experiment In terms of the number of animals used in biomedical research, the rat is regarded as the second laboratory animal. These mice are easily adapted to research methods. Today's laboratory rats are domesticated genera of Rattus norvegicus. In clinical trials, all tests were confirmed by the Ethics Committee of the Heart Center of the Azarbayjan Shahid Madani University. The animals used for this experiment were four adult rats weighing 283-328g obtained from the animal experiment center of Tabriz University. Experimental and biodiversity standards have been observed in all stages of surgery and experiments performed on live animals [ 21 , 22 ]. The rats were kept under this standard condition: -The rats are kept in Plexiglass cages with lattice metal caps and with dimensions of (24*15*35). In the cages, the ventilation operation was going well and the cages were cleaned every day. - The light period of the animals was carefully regulated. For example, 14 hours of lighting and 10 hours of darkness. - The temperature of the animals was also kept at standard temperature (25 ± 2°C). - Animal feeding was free and pelleted feed was used. - The animal's water container was made of glass or plastic and the rats always had access to safe and healthy water. -The humidity was about 55%. The rats daily consumed an average of 20 grams of food and a cup of water. Before creating the wound, the desired location for the wound is shaved and after that, the shaved place is disinfected. Ketamine has been used to anesthetize the animals that the dose of ketamine is 100 mg/kg body weight. 4. Result and discussion 4.1 FTIR Characterization FT–IR analysis of p-h-t is represented in Fig. 1 . The absorption bands at 2941 and 2864 cm − 1 are assigned to CH 2 asymmetric stretching and symmetric stretching for PCL and HEMA. The absorption band 1723 cm − 1 is related to the presence of the carbonyl group in PCL. According to Fig. 2 , due to the interaction of the carbonyl group with metal nanoparticles, the peak intensity of the carbonyl group in PCL has decreased. The absorption bands at1045, 1104, and 1239 cm − 1 are related to the stretching vibrations of the C—O—C (PCL). Bonds containing metal-oxygen are found in lower wavenumbers. Absorption peaks 455 and 406 cm − 1 indicate the presence of these bonds in the structure of P-H [ 23 , 24 ]. Also, due to the interaction of the hydroxyl group (HEMA) with PCL of this group in region 3200 cm − 1 has been removed. Figure 2 4.2 XRD Characterization Figure 3 shows the XRD pattern of P-H. According to the XRD spectrum pattern [ 25 , 26 , 27 ], the displacement peaks of PCL and HEMA from (21.31°, 23.71° and 33° respectively) to (21.48°, 23.84°), also the XRD spectrum pattern (Fig. 2 ) shows the removal of the peaks of TiO 2 (25.27°, 36.91°, 37.77°, 38.52°, 48.01°, 53.84°, 55.03°, 62.07°, 62.64°) and ZnO (31.76°,34.42°, 36.25°, 47.53°, 56.60°, 62.86°, 66.37°, 67.96°, 69.1°). By increasing the intensity and displacement peaks of PCL and HEMA, it can be concluded that nanoparticles (TiO 2 and ZnO) have interacted (interactions between hydrophilic TiO 2 , polar PCL, and HEMA) with PCL and HEMA. These results confirm the successful loading of nanoparticles in the polymer structure. Figure 3 4.3 contact angle test The contact angle value of p-H is shown in Fig. 3 . The contact angle value (131.64°) indicates the hydrophobic surface of this polymer, which is due to the load of HEMA and mineral nanoparticles (TiO 2 and ZnO) in the structure of the p-H. The presence of HEMA in the structure of the p-H increases the (CH 2 ) aliphatic part of the polymer and also the interaction of mineral nanoparticles with the hydroxyl group of HEMA reduces the polarity of this part. For these reasons, it shows the polymer exhibit hydrophobic surfaces. Figure 4 4.4 Mechanical properties The Young modulus or the modulus of elasticity in tension, is a mechanical property that measures the tensile stiffness of a solid material. It quantifies the relationship between tensile stress σ (force per unit area) and axial strain ε proportional deformation) in the linear elastic region of a material. The value Young modulus for p-H is 5.18 Mpa. This result shows the appropriate mechanical properties for this polymer. 4.5 In vivo experiment As shown in the picture (Fig. 5 ) how wounds appear in scaffolding and without scaffolding is shown. The wounds were examined on the first, third, and fifth days. [a] and [d] shows the result of examine at first day, all the experimental condition were same, the scaffold is placed on the[d]. [b] and [e] show the result of the experiment at 3rd day of treatment. The differences are obvious, [e] is a wound that fibrous scaffolding placed on it and it is clear that the scaffold is attached to the surface of the wound. In contrast, wound [b] has no scaffolding and there is evidence of white infection despite the disinfection of wounds. [c] and [f] show the result of the experiment on the 5th day of wound treatment. In the wound [f], the gaps are very small and it can be said that it has almost completely improved, but wound [c] compared to the wound [f] healed less. Results show that the use of this scaffold due to the use of antibacterial nanoparticles did not cause any inflammatory reactions. Wound area with scaffolding compared with scaffold-free wounds, was less and the wound healing process also happened faster. Figure 5 4.6 Investigation of antibacterial behavior of scaffolds Figure 6 show how wound dressings work against gram-negative and gram-positive bacteria. The results of antibacterial scaffold testing against different types of bacteria, gram-positive and gram-negative bacteria. Staphylococcus aureus )ATCC 25923) and Escherichia coli (ATTC 25922) are one of the most common pathogenic bacteria. As shown in the figure, no trace of bacterial growth is seen around scaffolding containing nanoparticles up to a radius of wound dress and this shows the antibacterial effect of TiO2 and ZnO nanoparticles.The results showed that the growth of gram-negative bacteria was more resistant to antibacterial nanoparticles. The reason for the greater resistance of gram-negative bacteria to nanoparticles can be attributed to the outer membrane, the structure of the bacterial wall, and the metabolism of this bacterium. Figure 6 4.7 Cell viability assay Figure 7 shows the growth characteristics of the cells in the3rd, 5th, and 7th days. As shown in the figure, cell growth on scaffolding containing 2.5% nanoparticles is more than other scaffolds. As the results show, cell growth is good even on scaffolds without any nanoparticles, this in itself demonstrates the interaction and compatibility of the cell with the polymers used Figure 8 Based on the normal distribution function of the data, F method has been used to obtain the equal variance evaluation. According to the statistical analysis done by Minitab, the p value obtained from the one way ANOVA is equal to zero. The zero p-value indicates the growth and differentiation of cells in day 3, 5 and 7. 4.8 Cell adhesion assay Examination of cell adhesion on polymer fibers can be obtained from SEM images. Due to the use of polyhydroxy ethyl methacrylate in the preparation of nanofibers, a very suitable three-dimensional space is provided for the growth and adhesion of cells. In this polymer scaffold, a strong hydration barrier is created that prevents the absorption of protein, and as a result, the cells do not adhere completely to the surface, which is created due to the strong hydrogen bond between the water molecules and the polymer [ 28 , 29 ]. The images obtained from the scanning electron microscopy show the morphology of the cells stretched toward the scaffold. At present, it can be said that electrospun pHEMA- PCL nanofibers have good biocompatibility. Figure 9 4.9 Bio-degradability assay The results of the weight loss test in Fig. 10 Showed that the process of weight loss of scaffolding was done with great intensity until the 15th day, but after the 15th day, this process was done at a very low speed. The sample containing 0% of zinc oxide and titanium oxide nanoparticles showed more weight loss than other samples Figure 10 Conclusion Optimal scaffolding is a pattern for tissue regeneration and plays a key role in shaping the final structure of engineered tissue and its ultimate function. The most important step in tissue engineering is choosing the right materials and the right way to make scaffolding. They must have several essential characteristics such as biocompatibility, biodegradability, and biological activity. Achieving success in the performance of skin substitutes is specifically based on how the cell behaves and the growth of the tissue, in which case it is necessary to use a bio-substance that can well provide the biological and mechanical properties of the skin tissue to provide nano topography to facilitate and modify cell exchanges with the environment, it is appropriate to provide nanoscale scaffolds, the production of which has attracted the attention of researchers in recent years. Different methods are used to prepare nanofibers, the most common of which are electrospinning, self-organizing, and fuzzy separation. Artificial polymers have mechanical properties superior to natural polymers and are easily processed. Polycaprolactone is a hydrophobic semi-crystalline polymer. Also, characteristics (C6H10O2) n Extraordinary mechanical molecular formula (mechanical flexibility), biocompatibility, it has low antigenicity, simple and easy processability, low melting point, and non-toxicity of the product resulting from its destruction. HEMA is a monomer used to make various polymers and is easily polymerized. HEMA and PCL nanofibers can support a wide range of cell types. One of the disadvantages of using caprolactone polymer is water repellency and consequently improper cell attachment. However, by combining this polymer with HEMA, a three-dimensional structure is created in the scaffold, in which the cell grows well in this three-dimensional environment. Studies have shown that cultured fibroblasts multiply three-dimensional faster than two-dimensional cultures. These differences appear to be due to the proximity of the cell space in the three-dimensional culture (culture on scaffolding) to the living environment. The results of the survival test in this study showed that the cells that grew on the scaffold of polymeric composition showed more absorption compared to the cells cultured on the scaffold of polycaprolactone. TiO 2 and ZnO loaded pHEMA-PCL scaffold via inexpensive electrospinning method was fabricated. Percentages of each nanoparticle, voltage, and the rate of electrospinning, affect the morphology of the scaffold. Any substance unique properties but a composite of these materials has acceptable features such as being antibacterial, non-toxic, biocompatibility, biodegradability, and porosity which have all the properties of a suitable scaffold. This scaffold contains 80% PCL, 15% HEMA, 2.5% TiO 2 and 2.5% ZnO Different percentages of NPS have been examined in this experiment but the growth and proliferation of fibroblast cells showed that the 2.5% of each nanoparticle is the best composition. The antibacterial effect of nanoparticles was investigated and the result was satisfying. Because of mentioned features, this scaffold can be used as a wound dress and skin tissue scaffold. Declarations Declaration of interests The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper. Author Contribution All authors reviewed the manuscript. References Díaz-Prado, S., Muiños-López, E., Hermida-Gómez, T., Cicione, C., Rendal-Vázquez, M.E., Fuentes-Boquete, I., de Toro, F.J. and Blanco, F.J., (2011). Human amniotic membrane as an alternative source of stem cells for regenerative medicine. Differentiation , 81 (3), pp.162-171. https://pubmed.ncbi.nlm.nih.gov/21339039/ Torres, E., Dominguez-Candela, I., Castello-Palacios, S., Vallés-Lluch, A., & Fombuena, V. (2020). Development and characterization of polyester and acrylate-based composites with hydroxyapatite and halloysite nanotubes for medical applications. Polymers , 12 (8), 1703. https://pubmed.ncbi.nlm.nih.gov/32751376/ Gomez, J.A., Lek, D., Song, I.H. and You, B.H., (2014). Study on stress evolution in the cooling process of micro hot embossing. International Journal of Mechanical and Materials Engineering , 9 (1), p.20. https://ijmme.springeropen.com/articles/10.1186/s40712-014-0020-9 RohitK.V., Varad N., Vinay A., Badal M., PritamP.P., RushikeshL.C., Apoorva S., Anubhav S., Vijay K. Y., Kamakshi P., Mahipal S.S., (2022). Zinc oxide (ZnO) nanoparticles: Synthesis properties and their forensic applications in latent fingerprints development, Materials Today: Proceeding, 69 (1) 36-41. https://www.sciencedirect.com/science/article/abs/pii/S2214785322052282 Huang, Z., Maness, P. C., Blake, D. M., Wolfrum, E. J., Smolinski, S. L., & Jacoby, W. A. (2000). Bactericidal mode of titanium dioxide photocatalysis. Journal of Photochemistry and Photobiology A: Chemistry , 130 (2-3), 163-170. https://www.sciencedirect.com/science/article/abs/pii/S1010603099002051 Pham, Q. P., Sharma, U., & Mikos, A. G. (2006). Electrospinning of polymeric nanofibers for tissue engineering applications: a review. Tissue engineering , 12 (5), 1197-1211. https://pubmed.ncbi.nlm.nih.gov/16771634/ Wu, T., Ding, M., Shi, C., Qiao, Y., Wang, P., Qiao, R., Zhong, J. (2020). Resorbable polymer electrospun nanofibers: History, shapes and application for tissue engineering. Chinese Chemical Letters , 31 (3), 617-625. https://www.sciencedirect.com/science/article/pii/S1001841719304152 Cavaliere, S., Subianto, S., Savych, I., Jones, D. J., & Rozière, J. (2011). Electrospinning: designed architectures for energy conversion and storage devices. Energy & Environmental Science , 4 (12), 4761-4785. https://pubs.rsc.org/en/content/articlelanding/2011/ee/c1ee02201f Gopal, R., Kaur, S., Ma, Z., Chan, C., Ramakrishna, S., & Matsuura, T. (2006). Electrospun nanofibrous filtration membrane. Journal of Membrane Science , 281 (1-2), 581-586. https://www.sciencedirect.com/science/article/abs/pii/S0376738806002651 Duan, G., Bagheri, A. R., Jiang, S., Golenser, J., Agarwal, S., & Greiner, A. (2017). Exploration of macroporous polymeric sponges as drug carriers. Biomacromolecules , 18 (10), 3215-3221. https://pubs.acs.org/doi/10.1021/acs.biomac.7b00852 Ryu, H. I., Koo, M. S., Kim, S., Kim, S., Park, Y. A., & Park, S. M. (2020). Uniform-thickness electrospun nanofiber mat production system based on real-time thickness measurement. Scientific reports , 10 (1), 1-10. https://www.nature.com/articles/s41598-020-77985-0 Zhang, C. L., & Yu, S. H. (2014). Nanoparticles meet electrospinning: recent advances and future prospects. Chemical Society Reviews , 43 (13), 4423-4448. https://pubs.rsc.org/en/content/articlelanding/2014/cs/c3cs60426h Solmaz Z., Khosro A., Younes B., Morteza B.(2021). Osteogenesis promotion of selenium-doped hydroxyapatite for application as bone scaffold. Biological Trace Element Research 199, 1802-1811. https://link.springer.com/article/10.1007/s12011-020-02309-2 Ren, L., Ozisik, R., Kotha, S. P., & Underhill, P. T. (2015). Highly efficient fabrication of polymer nanofiber assembly by centrifugal jet spinning: process and characterization. Macromolecules , 48 (8), 2593-2602. https://pubs.acs.org/doi/10.1021/acs.macromol.5b00292 Sridhar, R., Lakshminarayanan, R., Madhaiyan, K., Barathi, V. A., Lim, K. H. C., & Ramakrishna, S. (2015). Electrosprayed nanoparticles and electrospun nanofibers based on natural materials: applications in tissue regeneration, drug delivery and pharmaceuticals. Chemical Society Reviews , 44 (3), 790-814. https://pubmed.ncbi.nlm.nih.gov/25408245/ Beachley, V., & Wen, X. (2009). Effect of electrospinning parameters on the nanofiber diameter and length. Materials Science and Engineering: C , 29 (3), 663-668. https://www.sciencedirect.com/science/article/pii/S0928493108003226 De Bartolo, L., & Bader, A. (Eds.). (2013). Biomaterials for Stem Cell Therapy: State of Art and Vision for the Future. https://www.routledge.com/Biomaterials-for-Stem-Cell-Therapy-State-of-Art-and-Vision-for-the-Future/De-Bartolo-Bader/p/book/9781466576391 Kikuchi, A., & Okano, T. (2005). Nanostructured designs of biomedical materials: applications of cell sheet engineering to functional regenerative tissues and organs. Journal of Controlled Release , 101 (1-3), 69-84. https://pubmed.ncbi.nlm.nih.gov/15588895/ Ito, E., Suzuki, K., Yamato, M., Yokoyama, M., Sakurai, Y., & Okano, T. (1998). Active platelet movements on hydrophobic/hydrophilic microdomain‐structured surfaces. Journal of Biomedical Materials Research: An Official Journal of The Society for Biomaterials, The Japanese Society for Biomaterials, and the Australian Society for Biomaterials , 42 (1), 148-155. https://pubmed.ncbi.nlm.nih.gov/9740017/ Nojiri, C., Okano, T., Koyanagi, H., Nakahama, S., Park, K. D., & Kim, S. W. (1993). In vivo protein adsorption on polymers: Visualization of adsorbed proteins on vascular implants in dogs. Journal of Biomaterials Science, Polymer Edition , 4 (2), 75-88. https://pubmed.ncbi.nlm.nih.gov/1486066/ Robert S. (2016). 2016 Guidelines of the American Society of Mammalogists for the use of wild mammals in research and education. Journal of mammalogy, 97 (3), 663–688, https://academic.oup.com/jmammal/article/97/3/663/2459909 Griffin, J. L., Nicholls, A. W., Daykin, C. A., Heald, S., Keun, H. C., Schuppe-Koistinen, I., Robertson, D. (2007). Standard reporting requirements for biological samples in metabolomics experiments: mammalian/in vivo experiments. Metabolomics , 3 (3), 179-188. https://link.springer.com/article/10.1007/s11306-007-0077-z Fares, M. M., & Othman, A. A. (2009). Smart pH-sensitive alternating copolymers of (methylacrylamide-hydroxyethylmethacrylate); kinetic and physical properties. Journal of Macromolecular Science, Part A , 47 (1), 61-70. https://www.tandfonline.com/doi/abs/10.1080/10601320903399750 Gatti, S., Agostini, A., Ferrari, R., & Moscatelli, D. (2017). Synthesis and nanoprecipitation of HEMA-CLn based polymers for the production of biodegradable nanoparticles. Polymers , 9 (9), 389. https://pubmed.ncbi.nlm.nih.gov/30965689/ del Ángel-Sánchez, K., Borbolla-Torres, C. I., Palacios-Pineda, L. M., Ulloa-Castillo, N. A., & Elías-Zúñiga, A. (2019). Development, fabrication, and characterization of composite polycaprolactone membranes reinforced with TiO2 nanoparticles. Polymers , 11 (12), 1955. https://www.mdpi.com/2073-4360/11/12/1955 Arefi, M. R., & Rezaei-Zarchi, S. (2012). Synthesis of zinc oxide nanoparticles and their effect on the compressive strength and setting time of self-compacted concrete paste as cementitious composites. International journal of molecular sciences , 13 (4), 4340-4350. https://pubmed.ncbi.nlm.nih.gov/22605981/ Causa, F., Battista, E., Della Moglie, R., Guarnieri, D., Iannone, M., & Netti, P. A. (2010). Surface investigation on biomimetic materials to control cell adhesion: the case of RGD conjugation on PCL. Langmuir , 26 (12), 9875-9884. https://pubmed.ncbi.nlm.nih.gov/20349926/ Prime, K. L., & Whitesides, G. M. (1991). Self-assembled organic monolayers: model systems for studying adsorption of proteins at surfaces. Science , 1164-1167. https://www.science.org/doi/10.1126/science.252.5009.1164 Shahverdi, M., Seifi, S., Akbari, A., Mohammadi, K., Shamloo, A., & Movahhedy, M. R. (2022). Melt electrowriting of PLA, PCL, and composite PLA/PCL scaffolds for tissue engineering application. Scientific Reports , 12 (1), 19935. https://pubmed.ncbi.nlm.nih.gov/36402790/ Additional Declarations No competing interests reported. Cite Share Download PDF Status: Posted Version 1 posted You are reading this latest preprint version Research Square lets you share your work early, gain feedback from the community, and start making changes to your manuscript prior to peer review in a journal. As a division of Research Square Company, we’re committed to making research communication faster, fairer, and more useful. We do this by developing innovative software and high quality services for the global research community. Our growing team is made up of researchers and industry professionals working together to solve the most critical problems facing scientific publishing. Also discoverable on Platform About Our Team In Review Editorial Policies Advisory Board Help Center Resources Author Services Accessibility API Access RSS feed Manage Cookie Preferences © Research Square 2026 | ISSN 2693-5015 (online) Privacy Policy Terms of Service Do Not Sell My Personal Information {"props":{"pageProps":{"initialData":{"identity":"rs-3833998","acceptedTermsAndConditions":true,"allowDirectSubmit":true,"archivedVersions":[],"articleType":"Research Article","associatedPublications":[],"authors":[{"id":265615475,"identity":"0b3ead1b-5633-4d14-9362-f7118e95e63b","order_by":0,"name":"Fatemeh Samadian","email":"","orcid":"","institution":"Azarbaijan Shahid Madani University","correspondingAuthor":false,"prefix":"","firstName":"Fatemeh","middleName":"","lastName":"Samadian","suffix":""},{"id":265615476,"identity":"80dfa25e-02af-402c-83e1-473e5fd05f1e","order_by":1,"name":"Younes Beygi-Khosrowshahi","email":"data:image/png;base64,iVBORw0KGgoAAAANSUhEUgAAAZAAAAAyAQMAAABI0h/eAAAABlBMVEX///8AAABVwtN+AAAACXBIWXMAAA7EAAAOxAGVKw4bAAAA50lEQVRIiWNgGAWjYLACxgYgwcx8AEhKyJCihS0BpIWHBC0MPAZgkqBqg+O9Bx/+3GGTON+d5/OrGzUWPAzsh49uwKvlzLlkY94zaYkbD/Nus845BnQYT1raDbxabuSYSTO2HU7c2My7zTiHDahFgseMkBbznz/b/gO18DwzzvlHnBYzBt62A4nzmXmYH+e2EaFF8swZY2neM8nGG5jZzJhz+yR42Aj5he94j+HHnzvsZOf3H378OedbnRw/++FjeLUoHIDQjhsOMLBJgFhs+JSDgHwDhLYHMpg/EFI9CkbBKBgFIxMAAMTsS0MpO7ICAAAAAElFTkSuQmCC","orcid":"","institution":"Azarbaijan Shahid Madani University","correspondingAuthor":true,"prefix":"","firstName":"Younes","middleName":"","lastName":"Beygi-Khosrowshahi","suffix":""}],"badges":[],"createdAt":"2024-01-04 08:14:57","currentVersionCode":1,"declarations":"","doi":"10.21203/rs.3.rs-3833998/v1","doiUrl":"https://doi.org/10.21203/rs.3.rs-3833998/v1","draftVersion":[],"editorialEvents":[],"editorialNote":"","failedWorkflow":false,"files":[{"id":49327316,"identity":"fac41612-e807-4e93-89e3-acbcbc68f692","added_by":"auto","created_at":"2024-01-08 17:36:57","extension":"png","order_by":1,"title":"Figure 1","display":"","copyAsset":false,"role":"figure","size":289462,"visible":true,"origin":"","legend":"\u003cp\u003eThe synthesis of pHEMA/PCL loaded by Nano particles\u003c/p\u003e","description":"","filename":"floatimage1.png","url":"https://assets-eu.researchsquare.com/files/rs-3833998/v1/abb7d6df37368a078d045330.png"},{"id":49325769,"identity":"e16d622c-5f99-4fee-aa54-5e7f1a8da112","added_by":"auto","created_at":"2024-01-08 17:28:58","extension":"png","order_by":2,"title":"Figure 2","display":"","copyAsset":false,"role":"figure","size":184311,"visible":true,"origin":"","legend":"\u003cp\u003eFT-IR spectra of P-H.\u003c/p\u003e","description":"","filename":"floatimage2.png","url":"https://assets-eu.researchsquare.com/files/rs-3833998/v1/66a284c72adce654ab4dad0f.png"},{"id":49325764,"identity":"b84cc52b-ee25-49db-a5d9-c4db5ae13ffe","added_by":"auto","created_at":"2024-01-08 17:28:57","extension":"png","order_by":3,"title":"Figure 3","display":"","copyAsset":false,"role":"figure","size":106944,"visible":true,"origin":"","legend":"\u003cp\u003eX-ray diagram of a polymer scaffold containing nanoparticles\u003cstrong\u003e.\u003c/strong\u003e\u003c/p\u003e","description":"","filename":"floatimage3.png","url":"https://assets-eu.researchsquare.com/files/rs-3833998/v1/fb9b08944217c4469002b29f.png"},{"id":49327319,"identity":"3be88a94-58b7-4dea-890c-d92622915de0","added_by":"auto","created_at":"2024-01-08 17:36:58","extension":"png","order_by":4,"title":"Figure 4","display":"","copyAsset":false,"role":"figure","size":237849,"visible":true,"origin":"","legend":"\u003cp\u003eschematic of contact test\u003c/p\u003e","description":"","filename":"floatimage4.png","url":"https://assets-eu.researchsquare.com/files/rs-3833998/v1/c13916d4feec86d323ee1b74.png"},{"id":49325773,"identity":"0c8a65c6-d1e6-40c5-8e86-f92ce8f80729","added_by":"auto","created_at":"2024-01-08 17:28:58","extension":"png","order_by":5,"title":"Figure 5","display":"","copyAsset":false,"role":"figure","size":1525533,"visible":true,"origin":"","legend":"\u003cp\u003eThe figure shows the process of wound healing on different days and conditions with wound dressing and without wound dressing.\u003c/p\u003e","description":"","filename":"floatimage5.png","url":"https://assets-eu.researchsquare.com/files/rs-3833998/v1/8af2d7f34490a6408c13a8fe.png"},{"id":49325766,"identity":"8782b13b-b832-4dfe-a8ce-02bc6621d68c","added_by":"auto","created_at":"2024-01-08 17:28:57","extension":"png","order_by":6,"title":"Figure 6","display":"","copyAsset":false,"role":"figure","size":622150,"visible":true,"origin":"","legend":"\u003cp\u003eAntibacterial effect of selected samples for gram-negative bacteria and gram-positive bacteria\u003c/p\u003e","description":"","filename":"floatimage6.png","url":"https://assets-eu.researchsquare.com/files/rs-3833998/v1/5f7d67c2ad186347edd5ceeb.png"},{"id":49325774,"identity":"80a3abd1-88e8-474c-8b19-f8168ca25862","added_by":"auto","created_at":"2024-01-08 17:28:58","extension":"png","order_by":7,"title":"Figure 7","display":"","copyAsset":false,"role":"figure","size":18931,"visible":true,"origin":"","legend":"\u003cp\u003eShows cell growth on the third, fifth, and seventh days for samples with different nanoparticle percentages\u003cstrong\u003e.\u003c/strong\u003e\u003c/p\u003e","description":"","filename":"7.png","url":"https://assets-eu.researchsquare.com/files/rs-3833998/v1/cea06d818e81daf6bcb4aff1.png"},{"id":49325767,"identity":"1408459f-b096-4c8e-a751-0219651c9d18","added_by":"auto","created_at":"2024-01-08 17:28:58","extension":"png","order_by":8,"title":"Figure 8","display":"","copyAsset":false,"role":"figure","size":311664,"visible":true,"origin":"","legend":"\u003cp\u003e(A) show a linear relationship between cell proliferation and time (Day 3, 5 and 7) in Sample TiO2 and ZnO 2.5% and (B) shows Cell proliferation in Day 3, 5 and 7 in same sample.\u003c/p\u003e","description":"","filename":"floatimage7.png","url":"https://assets-eu.researchsquare.com/files/rs-3833998/v1/59539000f0163661097253f3.png"},{"id":49327317,"identity":"c269100a-fa03-4476-9c1b-d8b8e072f83c","added_by":"auto","created_at":"2024-01-08 17:36:58","extension":"png","order_by":9,"title":"Figure 9","display":"","copyAsset":false,"role":"figure","size":1190814,"visible":true,"origin":"","legend":"\u003cp\u003eShows the adhesion of the cell to the surface of the nanofibers that make up the scaffold.\u003c/p\u003e","description":"","filename":"floatimage8.png","url":"https://assets-eu.researchsquare.com/files/rs-3833998/v1/20f42253b6261340a1fb9013.png"},{"id":49325768,"identity":"30d4c1b7-dfd3-4fb2-8cde-889987b6d610","added_by":"auto","created_at":"2024-01-08 17:28:58","extension":"png","order_by":10,"title":"Figure 10","display":"","copyAsset":false,"role":"figure","size":20985,"visible":true,"origin":"","legend":"\u003cp\u003eWeight loss in day 3, 6, 9 12 and 15\u003c/p\u003e","description":"","filename":"10.png","url":"https://assets-eu.researchsquare.com/files/rs-3833998/v1/2437ac1a7b9b76488fc1d3e6.png"},{"id":50160836,"identity":"00ad9675-02dc-4898-9d41-a22e121f5b59","added_by":"auto","created_at":"2024-01-25 13:13:48","extension":"pdf","order_by":0,"title":"","display":"","copyAsset":false,"role":"manuscript-pdf","size":3654404,"visible":true,"origin":"","legend":"","description":"","filename":"manuscript.pdf","url":"https://assets-eu.researchsquare.com/files/rs-3833998/v1/125b58af-beec-45ff-9967-7cab6600f467.pdf"}],"financialInterests":"No competing interests reported.","formattedTitle":"Development of wound healing scaffold using ZnO and TiO2 nanoparticles","fulltext":[{"header":"1. INTRODUCTION","content":"\u003cp\u003eThe skin is the body's most important barrier against microorganisms and harmful substances. This barrier works best when healthy. Skin wounds can become infected and bacteria on the surface of the skin enter the body's bloodstream. Nowadays tissue engineering products promising for the treatment of skin lesions such as wounds and deep burns. Tissue engineering tries to restore the biological activities of damaged tissue to its original state by creating artificial tissue, and therefore plays a key role in wound healing and tissue replacement Interactions between biomaterials and tissues are highly dependent on the external surface structure of these substitutes. In this regard, the selection of the appropriate scaffold and cell plays a decisive role in achieving skin tissues that have similar characteristics in terms of histology and physiology to normal skin.\u003c/p\u003e \u003cp\u003eTissue engineering employs engineering and biological science principles and methods for the production and development of biological alternative Scaffolds, cells, growth factors and the main components of tissue engineering include polymers. The scaffold is a three-dimensional structure that is used as a framework to guide cells and it is a replacement for the extracellular matrix [\u003cspan citationid=\"CR1\" class=\"CitationRef\"\u003e1\u003c/span\u003e]. The structure of the scaffold must be possible for cells to adhere to it and it should be porous so when implanted on the body, the veins penetrate the scaffold and can feed the cells. One of the main characteristics of scaffolding is its degradability. The scaffold is gradually destroyed after the tissue is formed.\u003c/p\u003e \u003cp\u003ePolymers are usually the best materials for tissue scaffolds than ceramics because polymers have better plasticity. Among different polymers, polycaprolactone has excellent mechanical properties including good biodegradability, low anti-genius, simple processability, non-toxic products resulting from its destruction. [30]\u003c/p\u003e \u003cp\u003eBiodegradable electrospun PCL nanofibers, due to their advantages such as high surface to volume ratio in comparison with traditional scaffolds, are increasingly used for tissue engineering. Another material that is used in this article is poly hydroxyethyl methacrylate that is a nontoxic sterile polymer composed of 2-hydroxy ethyl methacrylate monomeric units. HEMA has a hydrophobic structure and hydrophilic cells are unable to adhere to the polymer surface. The cells are non-stick and suspended in 3D space between the environment and the polymer [\u003cspan citationid=\"CR2\" class=\"CitationRef\"\u003e2\u003c/span\u003e]. pHEMA has high solubility in organic solvents such as methanol and ethanol [\u003cspan citationid=\"CR3\" class=\"CitationRef\"\u003e3\u003c/span\u003e]. Furthermore, good mechanical stability, high biocompatibility, and physiological properties make pHEMA very useful used in biomedicine.\u003c/p\u003e \u003cp\u003eRecently, nanomaterials have been widely used in many fields due to the development and growth of nanotechnology. Zinc oxide and titanium oxide nanoparticles due to their anti-cancer, anti-bacterial, anti-inflammatory, and binding properties, are used in many fields like drug delivery, food additives, and tissue engineering. Zinc oxide has received much attention due to its unique surface and chemical properties and various functions in ultraviolet emitters, chemical sensors and piezoelectric devices, etc. Moreover, Titanium oxide, due to its special properties, has an amazing ability to destroy the walls of prokaryotes, such as Escherichia coli [\u003cspan citationid=\"CR4\" class=\"CitationRef\"\u003e4\u003c/span\u003e, \u003cspan citationid=\"CR5\" class=\"CitationRef\"\u003e5\u003c/span\u003e].\u003c/p\u003e \u003cp\u003eIn recent years, electrospinning with the ability to create polymeric nanofibers similar to the extracellular fibrous structure has attracted a lot of attraction. Electrospun nanofibers have many different applications in the fields of tissue engineering [\u003cspan citationid=\"CR6\" class=\"CitationRef\"\u003e6\u003c/span\u003e, \u003cspan citationid=\"CR7\" class=\"CitationRef\"\u003e7\u003c/span\u003e], energy storage [\u003cspan citationid=\"CR8\" class=\"CitationRef\"\u003e8\u003c/span\u003e], filtration [\u003cspan citationid=\"CR9\" class=\"CitationRef\"\u003e9\u003c/span\u003e], drug release[\u003cspan citationid=\"CR10\" class=\"CitationRef\"\u003e10\u003c/span\u003e], etc [\u003cspan citationid=\"CR11\" class=\"CitationRef\"\u003e11\u003c/span\u003e]. Combining nanoparticles and adding them to a polymer solution and electrospinning this solution and obtaining nanofibers containing nanoparticles is an up-to-date and interesting research field [\u003cspan citationid=\"CR12\" class=\"CitationRef\"\u003e12\u003c/span\u003e].\u003c/p\u003e \u003cp\u003eThe diameter of the fibers obtained from the electrospinning process may vary from ten nanometers to several micrometers. Polymeric or composite solutions and high voltage sources are used to prepare electrospun nanofibers [\u003cspan citationid=\"CR13\" class=\"CitationRef\"\u003e13\u003c/span\u003e, \u003cspan citationid=\"CR14\" class=\"CitationRef\"\u003e14\u003c/span\u003e]. One of the advantages of producing nanofibers by electrospin method is that the direction and size of the fibers can be controlled and also the rate and speed of fiber production can be controlled [\u003cspan citationid=\"CR15\" class=\"CitationRef\"\u003e15\u003c/span\u003e].\u003c/p\u003e \u003cp\u003eSimulation of the extracellular matrix fibrous arrangement in the body, high surface to volume ratio, and significant porosity are the most important benefits of electrospinning. Parameters such as polymer molecular weight, concentration, surface tension, viscosity and conductivity of polymer solution, voltage, injection rate, spinner and collector type, and environmental conditions control the electrospinning process [\u003cspan citationid=\"CR16\" class=\"CitationRef\"\u003e16\u003c/span\u003e].\u003c/p\u003e \u003cp\u003eIn this research, by using the conventional and inexpensive electrospinning method with using biodegradable and biocompatible polymers like polycaprolactone (PCL) and polyhydroxy ethyl methacrylate (pHEMA) and ceramic nanoparticles such as TiO\u003csub\u003e2\u003c/sub\u003e and ZnO, we tried to investigate the effect of the composite of these materials on the recovery time and absence of germs and infection at the wound site.\u003c/p\u003e"},{"header":"2. Method and Materials","content":"\u003cp\u003eThese materials have used in this experiment:\u003c/p\u003e \u003cp\u003eTiO2(Mw\u0026thinsp;=\u0026thinsp;79.866) and ZnO(Mw\u0026thinsp;=\u0026thinsp;81.40) nanoparticles, pcl(Mw\u0026thinsp;=\u0026thinsp;80 kDa), pHEMA(Mw=-kDa), phosphate buffer saline(PBS, ph\u0026thinsp;=\u0026thinsp;7.4), Roswell Park Memorial Institute Medium(RPMI medium), Fetal Bovine Serum(FBS, Gibco company), 3(4,5dimethylthiazol-2yl)-2,5diphenyltetrazolium bromide(MTT), Ketamine, 70% ethanol solution\u003c/p\u003e \u003cdiv id=\"Sec3\" class=\"Section2\"\u003e \u003ch2\u003e2.1 Polymer Synthesis\u003c/h2\u003e \u003cp\u003eThe p-H was synthesized by CL, HEMA, and nanoparticles (TiO2 and ZnO). First, Sn(Oct)2 (30 mg, 0.074 mmol( was mixed with HEMA (3.8 g, 0.029 mol) in a round-bottom flask at room temperature until Sn(Oct)2 is completely dissolved. Then, CL (10 g, 0.0877 mol) was heated up to 130\u0026deg;C in a stirred round-bottom flask. The HEMA/Sn(Oct)2 solution was then added to the flask, and the reaction was carried out for 2 h. The synthesis and nanoparticle loading procedure was shown in figure (1).\u003c/p\u003e \u003cp\u003eFigure\u0026nbsp;\u003cspan refid=\"Fig1\" class=\"InternalRef\"\u003e1\u003c/span\u003e\u003c/p\u003e \u003cp\u003e \u003c/p\u003e \u003c/div\u003e \u003cdiv id=\"Sec4\" class=\"Section2\"\u003e \u003ch2\u003e2.2 Fiber Preparation\u003c/h2\u003e \u003cp\u003eThe precursor solutions for electrospinning were prepared in a two-stage approach. First, a suspension of inorganic powder in the solvent mixture was achieved by dispersing 0.5 g of solid in 10 mL of chloroform, all being ultrasonicated for 5 min at 50% amplitude.\u003c/p\u003e \u003cp\u003eThen, 1.6 g of polymer was dissolved in the previously prepared suspension, which led to a final solution with 16% PCL and 5% inorganic powder; this was maintained under magnetic stirring for 24 h for PCL solubilization and general homogenization.\u003c/p\u003e \u003c/div\u003e \u003cdiv id=\"Sec5\" class=\"Section2\"\u003e \u003ch2\u003e2.3 Electrospinning process\u003c/h2\u003e \u003cp\u003eThe obtained solution was injected into a 5ml plastic syringe with a metallic needle and subjected to the electrospinning process. In this process electrical field was 19kv, the feeding rate was 0.5 ml/h and the distance from needle to collector was 18 cm.\u003c/p\u003e \u003c/div\u003e \u003cdiv id=\"Sec6\" class=\"Section2\"\u003e \u003ch2\u003e2.4 SEM characterization\u003c/h2\u003e \u003cp\u003eTo determine the characteristics of electrospun scaffolds, scanning electron microscopy (SEM) has used. To increase electrical conductivity, the surface of the scaffold was first covered with a thin coating with a thin layer of gold. The device used in this test is manufactured by Philips Netherlands and the model of the microscope is XL30.\u003c/p\u003e \u003c/div\u003e \u003cdiv id=\"Sec7\" class=\"Section2\"\u003e \u003ch2\u003e2.5 XRD Characterization\u003c/h2\u003e \u003cp\u003eAnother analysis used to study the Phase composition and crystallization of scaffolding is\u003c/p\u003e \u003cp\u003eX-Ray ((XRD) Philips TW 3710) diffraction.\u003c/p\u003e \u003cp\u003eX-ray diffraction analysis (XRD) has been used to investigate the composition of atoms in the structure of polymer crystals. After reviewing the results obtained from X-ray diffraction analysis, it can be seen that the nanoparticles are loaded into the structure of polymer fibers.\u003c/p\u003e \u003c/div\u003e \u003cdiv id=\"Sec8\" class=\"Section2\"\u003e \u003ch2\u003e2.6 FTIR Characterization\u003c/h2\u003e \u003cp\u003eTo comment on the loading of nanoparticles into polymer fibers and their reaction with polymer functional groups and to identify the functional groups present in the sample, a device Nicolet nexus 670 at a wavelength of 400-30000 cm\u003csup\u003e\u0026minus;\u0026thinsp;1\u003c/sup\u003e has been used.\u003c/p\u003e \u003c/div\u003e \u003cdiv id=\"Sec9\" class=\"Section2\"\u003e \u003ch2\u003e2.7 Contact Angle test\u003c/h2\u003e \u003cp\u003eGoniometer model CA-500A is used to measure the wettability of polymer nanofibers and the contact angle measurement model was sessile drop method. Distilled water is carefully poured on dry samples and in different cases, the contact angle is measured and photographed. The measurement is repeated several times for greater reliability and the contact angle is recorded when the error of the two data is less than 5%.\u003c/p\u003e \u003c/div\u003e \u003cdiv id=\"Sec10\" class=\"Section2\"\u003e \u003ch2\u003e2.8 mechanical properties\u003c/h2\u003e \u003cp\u003eIn addition to factors such as biocompatibility and porosity and biodegradability, mechanical properties are also the main features of a suitable scaffold. For this test, a 3*8 cm sample was used. Tension and strain testing device Z 010, Zwick/Roell, Ulm, Germany, has been used.\u003c/p\u003e \u003c/div\u003e \u003cdiv id=\"Sec11\" class=\"Section2\"\u003e \u003ch2\u003e2.9 Bio-Degradability assay\u003c/h2\u003e \u003cp\u003eTo evaluate the stability of polymeric scaffolds and measuring the rate of destruction in the body environment, hydrolytic and enzymatic biodegradability test was used. Therefore, the scaffolds were weighed (dry weight) and placed in a phosphate-buffered saline solution\u003c/p\u003e \u003cp\u003e(PBS) containing 4 mg/ml trypsin enzyme for one month. During 15 days of biodegradability testing, each week the scaffolds were dried in a freeze dryer and their dry weight was measured. It should be noted that the scaffolding medium was changed weekly and by the end of the fourth week, the remaining mass percentage of the scaffolds was obtained from the following equation. The test was repeated three times for each sample to obtain the mean and standard deviation.\u003c/p\u003e \u003cp\u003eWeight lost (%) = \u003cspan class=\"InlineEquation\"\u003e\u003cspan class=\"mathinline\"\u003e\\(\\frac{Wi-Wf}{Wi}\\times\\)\u003c/span\u003e\u003c/span\u003e100\u003c/p\u003e \u003cp\u003eW\u003csub\u003ei\u003c/sub\u003e is the weight of nanoparticle loaded scaffold in dry state and W\u003csub\u003ef\u003c/sub\u003e is the final wet weight.\u003c/p\u003e \u003c/div\u003e"},{"header":"3. Biocompatibility analysis","content":"\u003cdiv id=\"Sec13\" class=\"Section2\"\u003e\n \u003ch2\u003e3.1 Cell culture\u003c/h2\u003e\n \u003cp\u003eSkin fibroblast cells were cultured in a tissue culture flask and containing RPMI (cell culture media),1% antibiotic, and 10% FBS (fetal bovine serum), then incubated at 37\u0026deg;C, 5% CO2 and 90% humidity.\u003c/p\u003e\n \u003cp\u003eDuring this experiment, cell culture media was changed every 2 days.\u003c/p\u003e\n\u003c/div\u003e\n\u003cdiv id=\"Sec14\" class=\"Section2\"\u003e\n \u003ch2\u003e3.2 Cell viability assay\u003c/h2\u003e\n \u003cp\u003eThis experiment is conducted in both direct and indirect ways. For analysis of proliferation and viability of cells, 4\u0026times;10\u003csup\u003e4\u003c/sup\u003e cells (mouse fibroblast cells, CRL-2017) were seeded in 24 well plates in the presence of sterilized fibrous scaffold, and then RPMI media was added and 48 hours stayed at CO2 incubator under 90% air condition and 5% CO2 at 37 C. After 48 h, the MTT solution was added into each well and kept in dark condition inside of the CO2 incubator. After spending 8 h, DMSO was added to dissolve formazan crystals. UV spectrometer at a wavelength of 570 nm was used to measure absorbance.\u003c/p\u003e\n\u003c/div\u003e\n\u003cdiv id=\"Sec15\" class=\"Section2\"\u003e\n \u003ch2\u003e3.3 Cell adhesion assay\u003c/h2\u003e\n \u003cp\u003eFor measuring cell attachment, scaffolds (sterilized scaffold) were put into 6 well plates then 4\u0026times;10\u003csup\u003e4\u003c/sup\u003e cells per well and media was added in each well. The sample was incubated for 8 hours and then the media was changed with new RPMI media. In this step, the sample was washed with PBS solution and glutaraldehyde was used as a fixator.\u003c/p\u003e\n \u003cp\u003eAfter that fixator was removed, samples were washed with deionized water. The attached cells were observed with electron scanning microscopy (SEM). There may be three modes in the interaction between the cell and the polymer scaffold [\u003cspan class=\"CitationRef\"\u003e17\u003c/span\u003e, \u003cspan class=\"CitationRef\"\u003e18\u003c/span\u003e].\u003c/p\u003e\n \u003cp\u003eIn the first type, the interaction between the cell and the polymer scaffold is non-adhesive, in other words, no interaction occurs and in the second type, the cells interact with each other but can easily separate. This type of adhesion is called inactive adhesion. In the second type, the surface response is controlled by physicochemical interactions between the polymer surface, adsorbed proteins, and adhesive cells [\u003cspan class=\"CitationRef\"\u003e19\u003c/span\u003e, \u003cspan class=\"CitationRef\"\u003e20\u003c/span\u003e]. In the third type, the cells interact spontaneously and strongly and adhere firmly to the surface of the polymer.\u003c/p\u003e\n\u003c/div\u003e\n\u003cdiv id=\"Sec16\" class=\"Section2\"\u003e\n \u003ch2\u003e3.4 Antibacterial properties\u003c/h2\u003e\n \u003cp\u003eAs mentioned earlier, TiO2 and ZnO nanoparticles have antibacterial properties that can be examined using gram-negative and gram-positive bacteria due to agar diffusion. For this test Escherichia coli (E. coli) from the Enterobacteriaceae family as gram-negative bacteria and Staphylococcus aureus from Staphylococcaceae family as gram-positive bacteria are used. The diameter of the circular scaffolds is one centimeter and we test the scaffolds with 2.5% and a scaffold without nanoparticles.\u003c/p\u003e\n \u003cp\u003eNutrient agar media was poured into a bacterial culture plate and after that media dried, bacteria cultured on this. Then we place the samples on the plate and after that plate was kept in an incubator at 37 C for 24 h. Lack of bacterial growth around the samples is evident that has shown in pictures.\u003c/p\u003e\n\u003c/div\u003e\n\u003cdiv id=\"Sec17\" class=\"Section2\"\u003e\n \u003ch2\u003e3.5 In vivo experiment\u003c/h2\u003e\n \u003cp\u003eIn terms of the number of animals used in biomedical research, the rat is regarded as the second laboratory animal. These mice are easily adapted to research methods. Today\u0026apos;s laboratory rats are domesticated genera of Rattus norvegicus. In clinical trials, all tests were confirmed by the Ethics Committee of the Heart Center of the Azarbayjan Shahid Madani University.\u003c/p\u003e\n \u003cp\u003eThe animals used for this experiment were four adult rats weighing 283-328g obtained from the animal experiment center of Tabriz University. Experimental and biodiversity standards have been observed in all stages of surgery and experiments performed on live animals [\u003cspan class=\"CitationRef\"\u003e21\u003c/span\u003e, \u003cspan class=\"CitationRef\"\u003e22\u003c/span\u003e].\u003c/p\u003e\n \u003cp\u003eThe rats were kept under this standard condition:\u003c/p\u003e\n \u003cp\u003e-The rats are kept in Plexiglass cages with lattice metal caps and with dimensions of (24*15*35). In the cages, the ventilation operation was going well and the cages were cleaned every day.\u003c/p\u003e\n \u003cp\u003e- The light period of the animals was carefully regulated. For example, 14 hours of lighting and 10 hours of darkness.\u003c/p\u003e\n \u003cp\u003e- The temperature of the animals was also kept at standard temperature (25\u0026thinsp;\u0026plusmn;\u0026thinsp;2\u0026deg;C).\u003c/p\u003e\n \u003cp\u003e- Animal feeding was free and pelleted feed was used.\u003c/p\u003e\n \u003cp\u003e- The animal\u0026apos;s water container was made of glass or plastic and the rats always had access to safe and healthy water.\u003c/p\u003e\n \u003cp\u003e-The humidity was about 55%.\u003c/p\u003e\n \u003cp\u003eThe rats daily consumed an average of 20 grams of food and a cup of water.\u003c/p\u003e\n \u003cp\u003eBefore creating the wound, the desired location for the wound is shaved and after that, the shaved place is disinfected.\u003c/p\u003e\n \u003cp\u003eKetamine has been used to anesthetize the animals that the dose of ketamine is 100 mg/kg body weight.\u003c/p\u003e\n\u003c/div\u003e"},{"header":"4. Result and discussion","content":"\u003cdiv id=\"Sec19\"\u003e\n \u003ch2\u003e4.1 FTIR Characterization\u003c/h2\u003e\n \u003cp\u003eFT–IR analysis of p-h-t is represented in Fig.\u0026nbsp;\u003cspan\u003e1\u003c/span\u003e. The absorption bands at 2941 and 2864 cm\u003csup\u003e− 1\u003c/sup\u003e are assigned to CH\u003csub\u003e2\u003c/sub\u003e asymmetric stretching and symmetric stretching for PCL and HEMA. The absorption band 1723 cm\u003csup\u003e− 1\u003c/sup\u003e is related to the presence of the carbonyl group in PCL. According to Fig.\u0026nbsp;\u003cspan\u003e2\u003c/span\u003e, due to the interaction of the carbonyl group with metal nanoparticles, the peak intensity of the carbonyl group in PCL has decreased. The absorption bands at1045, 1104, and 1239 cm\u003csup\u003e− 1\u003c/sup\u003e are related to the stretching vibrations of the C—O—C (PCL). Bonds containing metal-oxygen are found in lower wavenumbers. Absorption peaks 455 and 406 cm\u003csup\u003e− 1\u003c/sup\u003e indicate the presence of these bonds in the structure of P-H [\u003cspan\u003e23\u003c/span\u003e, \u003cspan\u003e24\u003c/span\u003e]. Also, due to the interaction of the hydroxyl group (HEMA) with PCL of this group in region 3200 cm\u003csup\u003e− 1\u003c/sup\u003e has been removed.\u003c/p\u003e\n \u003cp\u003eFigure\u0026nbsp;\u003cspan\u003e2\u003c/span\u003e\u003c/p\u003e\n\u003c/div\u003e\n\u003cdiv id=\"Sec20\"\u003e\n \u003ch2\u003e4.2 XRD Characterization\u003c/h2\u003e\n \u003cp\u003eFigure \u003cspan\u003e3\u003c/span\u003e shows the XRD pattern of P-H. According to the XRD spectrum pattern [\u003cspan\u003e25\u003c/span\u003e, \u003cspan\u003e26\u003c/span\u003e, \u003cspan\u003e27\u003c/span\u003e], the displacement peaks of PCL and HEMA from (21.31°, 23.71° and 33° respectively) to (21.48°, 23.84°), also the XRD spectrum pattern (Fig.\u0026nbsp;\u003cspan\u003e2\u003c/span\u003e) shows the removal of the peaks of TiO\u003csub\u003e2\u003c/sub\u003e (25.27°, 36.91°, 37.77°, 38.52°, 48.01°, 53.84°, 55.03°, 62.07°, 62.64°) and ZnO (31.76°,34.42°, 36.25°, 47.53°, 56.60°, 62.86°, 66.37°, 67.96°, 69.1°). By increasing the intensity and displacement peaks of PCL and HEMA, it can be concluded that nanoparticles (TiO\u003csub\u003e2\u003c/sub\u003e and ZnO) have interacted (interactions between hydrophilic TiO\u003csub\u003e2\u003c/sub\u003e, polar PCL, and HEMA) with PCL and HEMA. These results confirm the successful loading of nanoparticles in the polymer structure.\u003c/p\u003e\n \u003cp\u003eFigure\u0026nbsp;\u003cspan\u003e3\u003c/span\u003e\u003c/p\u003e\n\u003c/div\u003e\n\u003cdiv id=\"Sec21\"\u003e\n \u003ch2\u003e4.3 contact angle test\u003c/h2\u003e\n \u003cp\u003eThe contact angle value of p-H is shown in Fig.\u0026nbsp;\u003cspan\u003e3\u003c/span\u003e. The contact angle value (131.64°) indicates the hydrophobic surface of this polymer, which is due to the load of HEMA and mineral nanoparticles (TiO\u003csub\u003e2\u003c/sub\u003e and ZnO) in the structure of the p-H. The presence of HEMA in the structure of the p-H increases the (CH\u003csub\u003e2\u003c/sub\u003e) aliphatic part of the polymer and also the interaction of mineral nanoparticles with the hydroxyl group of HEMA reduces the polarity of this part. For these reasons, it shows the polymer exhibit hydrophobic surfaces.\u003c/p\u003e\n \u003cp\u003eFigure\u0026nbsp;\u003cspan\u003e4\u003c/span\u003e\u003c/p\u003e\n\u003c/div\u003e\n\u003cdiv id=\"Sec22\"\u003e\n \u003ch2\u003e4.4 Mechanical properties\u003c/h2\u003e\n \u003cp\u003eThe Young modulus or the modulus of elasticity in tension, is a mechanical property that measures the tensile stiffness of a solid material. It quantifies the relationship between tensile stress σ (force per unit area) and axial strain ε proportional deformation) in the linear elastic region of a material. The value Young modulus for p-H is 5.18 Mpa. This result shows the appropriate mechanical properties for this polymer.\u003c/p\u003e\n\u003c/div\u003e\n\u003cdiv id=\"Sec23\"\u003e\n \u003ch2\u003e4.5 In vivo experiment\u003c/h2\u003e\n \u003cp\u003eAs shown in the picture (Fig.\u0026nbsp;\u003cspan\u003e5\u003c/span\u003e) how wounds appear in scaffolding and without scaffolding is shown. The wounds were examined on the first, third, and fifth days.\u003c/p\u003e\n \u003cp\u003e\u003cspan\u003e[a] and [d] shows the result of examine at first day, all the experimental condition were same, the scaffold is placed on the[d]. [b] and [e] show the result of the experiment at 3rd day of treatment. The differences are obvious, [e] is a wound that fibrous scaffolding placed on it and it is clear that the scaffold is attached to the surface of the wound. In contrast, wound [b] has no scaffolding and there is evidence of white infection despite the disinfection of wounds.\u003cbr\u003e\u003c/span\u003e \u003cspan\u003e[c] and [f] show the result of the experiment on the 5th day of wound treatment. In the wound [f], the gaps are very small and it can be said that it has almost completely improved, but wound [c] compared to the wound [f] healed less. Results show that the use of this scaffold due to the use of antibacterial nanoparticles did not cause any inflammatory reactions. Wound area with scaffolding compared with scaffold-free wounds, was less and the wound healing process also happened faster.\u003cbr\u003e\u003c/span\u003e\u003c/p\u003e\n \u003cp\u003eFigure\u0026nbsp;\u003cspan\u003e5\u003c/span\u003e\u003c/p\u003e\n\u003c/div\u003e\n\u003cdiv id=\"Sec24\"\u003e\n \u003ch2\u003e4.6 Investigation of antibacterial behavior of scaffolds\u003c/h2\u003e\n \u003cp\u003eFigure\u003cspan\u003e6\u003c/span\u003e show how wound dressings work against gram-negative and gram-positive bacteria. The results of antibacterial scaffold testing against different types of bacteria, gram-positive and gram-negative bacteria. Staphylococcus aureus )ATCC 25923) and Escherichia coli (ATTC 25922) are one of the most common pathogenic bacteria.\u003c/p\u003e\n \u003cp\u003eAs shown in the figure, no trace of bacterial growth is seen around scaffolding containing nanoparticles up to a radius of wound dress and this shows the antibacterial effect of TiO2 and ZnO nanoparticles.The results showed that the growth of gram-negative bacteria was more resistant to antibacterial nanoparticles. The reason for the greater resistance of gram-negative bacteria to nanoparticles can be attributed to the outer membrane, the structure of the bacterial wall, and the metabolism of this bacterium.\u003c/p\u003e\n \u003cp\u003eFigure\u0026nbsp;\u003cspan\u003e6\u003c/span\u003e\u003c/p\u003e\n\u003c/div\u003e\n\u003cdiv id=\"Sec25\"\u003e\n \u003ch2\u003e4.7 Cell viability assay\u003c/h2\u003e\n \u003cp\u003eFigure \u003cspan\u003e7\u003c/span\u003e shows the growth characteristics of the cells in the3rd, 5th, and 7th days. As shown in the figure, cell growth on scaffolding containing 2.5% nanoparticles is more than other scaffolds. As the results show, cell growth is good even on scaffolds without any nanoparticles, this in itself demonstrates the interaction and compatibility of the cell with the polymers used\u003c/p\u003e\n \u003cp\u003eFigure\u0026nbsp;\u003cspan\u003e8\u003c/span\u003e\u003c/p\u003e\n \u003cp\u003eBased on the normal distribution function of the data, F method has been used to obtain the equal variance evaluation. According to the statistical analysis done by Minitab, the p value obtained from the one way ANOVA is equal to zero. The zero p-value indicates the growth and differentiation of cells in day 3, 5 and 7.\u003c/p\u003e\n\u003c/div\u003e\n\u003cdiv id=\"Sec26\"\u003e\n \u003ch2\u003e4.8 Cell adhesion assay\u003c/h2\u003e\n \u003cp\u003eExamination of cell adhesion on polymer fibers can be obtained from SEM images. Due to the use of polyhydroxy ethyl methacrylate in the preparation of nanofibers, a very suitable three-dimensional space is provided for the growth and adhesion of cells. In this polymer scaffold, a strong hydration barrier is created that prevents the absorption of protein, and as a result, the cells do not adhere completely to the surface, which is created due to the strong hydrogen bond between the water molecules and the polymer [\u003cspan\u003e28\u003c/span\u003e, \u003cspan\u003e29\u003c/span\u003e].\u003c/p\u003e\n \u003cp\u003eThe images obtained from the scanning electron microscopy show the morphology of the cells stretched toward the scaffold. At present, it can be said that electrospun pHEMA- PCL nanofibers have good biocompatibility.\u003c/p\u003e\n \u003cp\u003eFigure\u0026nbsp;\u003cspan\u003e9\u003c/span\u003e\u003c/p\u003e\n\u003c/div\u003e\n\u003cdiv id=\"Sec27\"\u003e\n \u003ch2\u003e4.9 Bio-degradability assay\u003c/h2\u003e\n \u003cp\u003eThe results of the weight loss test in Fig.\u0026nbsp;\u003cspan\u003e10\u003c/span\u003e Showed that the process of weight loss of scaffolding was done with great intensity until the 15th day, but after the 15th day, this process was done at a very low speed. The sample containing 0% of zinc oxide and titanium oxide nanoparticles showed more weight loss than other samples\u003c/p\u003e\n \u003cp\u003eFigure\u0026nbsp;\u003cspan\u003e10\u003c/span\u003e\u003c/p\u003e\n \n \n \n \n \n\u003c/div\u003e"},{"header":"Conclusion","content":"\u003cp\u003eOptimal scaffolding is a pattern for tissue regeneration and plays a key role in shaping the final structure of engineered tissue and its ultimate function. The most important step in tissue engineering is choosing the right materials and the right way to make scaffolding. They must have several essential characteristics such as biocompatibility, biodegradability, and biological activity. Achieving success in the performance of skin substitutes is specifically based on how the cell behaves and the growth of the tissue, in which case it is necessary to use a bio-substance that can well provide the biological and mechanical properties of the skin tissue to provide nano topography to facilitate and modify cell exchanges with the environment, it is appropriate to provide nanoscale scaffolds, the production of which has attracted the attention of researchers in recent years. Different methods are used to prepare nanofibers, the most common of which are electrospinning, self-organizing, and fuzzy separation. Artificial polymers have mechanical properties superior to natural polymers and are easily processed. Polycaprolactone is a hydrophobic semi-crystalline polymer. Also, characteristics (C6H10O2) n Extraordinary mechanical molecular formula (mechanical flexibility), biocompatibility, it has low antigenicity, simple and easy processability, low melting point, and non-toxicity of the product resulting from its destruction. HEMA is a monomer used to make various polymers and is easily polymerized. HEMA and PCL nanofibers can support a wide range of cell types. One of the disadvantages of using caprolactone polymer is water repellency and consequently improper cell attachment. However, by combining this polymer with HEMA, a three-dimensional structure is created in the scaffold, in which the cell grows well in this three-dimensional environment. Studies have shown that cultured fibroblasts multiply three-dimensional faster than two-dimensional cultures. These differences appear to be due to the proximity of the cell space in the three-dimensional culture (culture on scaffolding) to the living environment. The results of the survival test in this study showed that the cells that grew on the scaffold of polymeric composition showed more absorption compared to the cells cultured on the scaffold of polycaprolactone.\u003c/p\u003e\u003cp\u003eTiO\u003csub\u003e2\u003c/sub\u003e and ZnO loaded pHEMA-PCL scaffold via inexpensive electrospinning method was fabricated. Percentages of each nanoparticle, voltage, and the rate of electrospinning, affect the morphology of the scaffold. Any substance unique properties but a composite of these materials has acceptable features such as being antibacterial, non-toxic, biocompatibility, biodegradability, and porosity which have all the properties of a suitable scaffold.\u003c/p\u003e\u003cp\u003eThis scaffold contains 80% PCL, 15% HEMA, 2.5% TiO\u003csub\u003e2\u003c/sub\u003e and 2.5% ZnO Different percentages of NPS have been examined in this experiment but the growth and proliferation of fibroblast cells showed that the 2.5% of each nanoparticle is the best composition.\u003c/p\u003e\u003cp\u003eThe antibacterial effect of nanoparticles was investigated and the result was satisfying. Because of mentioned features, this scaffold can be used as a wound dress and skin tissue scaffold.\u003c/p\u003e"},{"header":"Declarations","content":"\u003cp\u003e\u003cstrong\u003eDeclaration of interests\u003c/strong\u003e\u003c/p\u003e\n\u003cp\u003eThe authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.\u003c/p\u003e\u003ch2\u003eAuthor Contribution\u003c/h2\u003e\u003cp\u003eAll authors reviewed the manuscript.\u003c/p\u003e"},{"header":"References","content":"\u003col\u003e\n\u003cli\u003eD\u0026iacute;az-Prado, S., Mui\u0026ntilde;os-L\u0026oacute;pez, E., Hermida-G\u0026oacute;mez, T., Cicione, C., Rendal-V\u0026aacute;zquez, M.E., Fuentes-Boquete, I., de Toro, F.J. and Blanco, F.J., (2011). Human amniotic membrane as an alternative source of stem cells for regenerative medicine. \u003cem\u003eDifferentiation\u003c/em\u003e, \u003cem\u003e81\u003c/em\u003e(3), pp.162-171. https://pubmed.ncbi.nlm.nih.gov/21339039/\u003c/li\u003e\n\u003cli\u003eTorres, E., Dominguez-Candela, I., Castello-Palacios, S., Vall\u0026eacute;s-Lluch, A., \u0026amp; Fombuena, V. (2020). Development and characterization of polyester and acrylate-based composites with hydroxyapatite and halloysite nanotubes for medical applications. \u003cem\u003ePolymers\u003c/em\u003e, \u003cem\u003e12\u003c/em\u003e(8), 1703. https://pubmed.ncbi.nlm.nih.gov/32751376/\u003c/li\u003e\n\u003cli\u003eGomez, J.A., Lek, D., Song, I.H. and You, B.H., (2014). Study on stress evolution in the cooling process of micro hot embossing. \u003cem\u003eInternational Journal of Mechanical and Materials Engineering\u003c/em\u003e, \u003cem\u003e9\u003c/em\u003e(1), p.20. https://ijmme.springeropen.com/articles/10.1186/s40712-014-0020-9\u003c/li\u003e\n\u003cli\u003eRohitK.V., Varad N., Vinay A., Badal M., PritamP.P., RushikeshL.C., Apoorva S., Anubhav S., Vijay K. Y., Kamakshi P., Mahipal S.S., (2022). Zinc oxide (ZnO) nanoparticles: Synthesis properties and their forensic applications in latent fingerprints development, \u003cem\u003eMaterials Today: Proceeding, \u003c/em\u003e69 (1) 36-41.\u003cem\u003e \u003c/em\u003ehttps://www.sciencedirect.com/science/article/abs/pii/S2214785322052282\u003cem\u003e \u003c/em\u003e \u003c/li\u003e\n\u003cli\u003eHuang, Z., Maness, P. C., Blake, D. M., Wolfrum, E. J., Smolinski, S. L., \u0026amp; Jacoby, W. A. (2000). Bactericidal mode of titanium dioxide photocatalysis. \u003cem\u003eJournal of Photochemistry and Photobiology A: Chemistry\u003c/em\u003e, \u003cem\u003e130\u003c/em\u003e(2-3), 163-170. https://www.sciencedirect.com/science/article/abs/pii/S1010603099002051\u003c/li\u003e\n\u003cli\u003ePham, Q. P., Sharma, U., \u0026amp; Mikos, A. G. (2006). Electrospinning of polymeric nanofibers for tissue engineering applications: a review. \u003cem\u003eTissue engineering\u003c/em\u003e, \u003cem\u003e12\u003c/em\u003e(5), 1197-1211. https://pubmed.ncbi.nlm.nih.gov/16771634/\u003c/li\u003e\n\u003cli\u003eWu, T., Ding, M., Shi, C., Qiao, Y., Wang, P., Qiao, R., Zhong, J. (2020). Resorbable polymer electrospun nanofibers: History, shapes and application for tissue engineering. \u003cem\u003eChinese Chemical Letters\u003c/em\u003e, \u003cem\u003e31\u003c/em\u003e(3), 617-625. https://www.sciencedirect.com/science/article/pii/S1001841719304152\u003c/li\u003e\n\u003cli\u003eCavaliere, S., Subianto, S., Savych, I., Jones, D. J., \u0026amp; Rozi\u0026egrave;re, J. (2011). Electrospinning: designed architectures for energy conversion and storage devices. \u003cem\u003eEnergy \u0026amp; Environmental Science\u003c/em\u003e, \u003cem\u003e4\u003c/em\u003e(12), 4761-4785. https://pubs.rsc.org/en/content/articlelanding/2011/ee/c1ee02201f\u003c/li\u003e\n\u003cli\u003eGopal, R., Kaur, S., Ma, Z., Chan, C., Ramakrishna, S., \u0026amp; Matsuura, T. (2006). Electrospun nanofibrous filtration membrane. \u003cem\u003eJournal of Membrane Science\u003c/em\u003e, \u003cem\u003e281\u003c/em\u003e(1-2), 581-586. https://www.sciencedirect.com/science/article/abs/pii/S0376738806002651\u003c/li\u003e\n\u003cli\u003eDuan, G., Bagheri, A. R., Jiang, S., Golenser, J., Agarwal, S., \u0026amp; Greiner, A. (2017). Exploration of macroporous polymeric sponges as drug carriers. \u003cem\u003eBiomacromolecules\u003c/em\u003e, \u003cem\u003e18\u003c/em\u003e(10), 3215-3221. https://pubs.acs.org/doi/10.1021/acs.biomac.7b00852\u003c/li\u003e\n\u003cli\u003eRyu, H. I., Koo, M. S., Kim, S., Kim, S., Park, Y. A., \u0026amp; Park, S. M. (2020). Uniform-thickness electrospun nanofiber mat production system based on real-time thickness measurement. \u003cem\u003eScientific reports\u003c/em\u003e, \u003cem\u003e10\u003c/em\u003e(1), 1-10. https://www.nature.com/articles/s41598-020-77985-0\u003c/li\u003e\n\u003cli\u003eZhang, C. L., \u0026amp; Yu, S. H. (2014). Nanoparticles meet electrospinning: recent advances and future prospects. \u003cem\u003eChemical Society Reviews\u003c/em\u003e, \u003cem\u003e43\u003c/em\u003e(13), 4423-4448. https://pubs.rsc.org/en/content/articlelanding/2014/cs/c3cs60426h \u003c/li\u003e\n\u003cli\u003eSolmaz Z., Khosro A., Younes B., Morteza B.(2021). Osteogenesis promotion of selenium-doped hydroxyapatite for application as bone scaffold. \u003cem\u003eBiological Trace Element Research\u003c/em\u003e 199, 1802-1811. https://link.springer.com/article/10.1007/s12011-020-02309-2 \u003c/li\u003e\n\u003cli\u003eRen, L., Ozisik, R., Kotha, S. P., \u0026amp; Underhill, P. T. (2015). Highly efficient fabrication of polymer nanofiber assembly by centrifugal jet spinning: process and characterization. \u003cem\u003eMacromolecules\u003c/em\u003e, \u003cem\u003e48\u003c/em\u003e(8), 2593-2602. https://pubs.acs.org/doi/10.1021/acs.macromol.5b00292 \u003c/li\u003e\n\u003cli\u003eSridhar, R., Lakshminarayanan, R., Madhaiyan, K., Barathi, V. A., Lim, K. H. C., \u0026amp; Ramakrishna, S. (2015). Electrosprayed nanoparticles and electrospun nanofibers based on natural materials: applications in tissue regeneration, drug delivery and pharmaceuticals. \u003cem\u003eChemical Society Reviews\u003c/em\u003e, \u003cem\u003e44\u003c/em\u003e(3), 790-814. https://pubmed.ncbi.nlm.nih.gov/25408245/ \u003c/li\u003e\n\u003cli\u003eBeachley, V., \u0026amp; Wen, X. (2009). Effect of electrospinning parameters on the nanofiber diameter and length. \u003cem\u003eMaterials Science and Engineering: C\u003c/em\u003e, \u003cem\u003e29\u003c/em\u003e(3), 663-668. https://www.sciencedirect.com/science/article/pii/S0928493108003226 \u003c/li\u003e\n\u003cli\u003eDe Bartolo, L., \u0026amp; Bader, A. (Eds.). (2013). Biomaterials for Stem Cell Therapy: State of Art and Vision for the Future. https://www.routledge.com/Biomaterials-for-Stem-Cell-Therapy-State-of-Art-and-Vision-for-the-Future/De-Bartolo-Bader/p/book/9781466576391 \u003c/li\u003e\n\u003cli\u003eKikuchi, A., \u0026amp; Okano, T. (2005). Nanostructured designs of biomedical materials: applications of cell sheet engineering to functional regenerative tissues and organs. \u003cem\u003eJournal of Controlled Release\u003c/em\u003e, \u003cem\u003e101\u003c/em\u003e(1-3), 69-84. https://pubmed.ncbi.nlm.nih.gov/15588895/ \u003c/li\u003e\n\u003cli\u003eIto, E., Suzuki, K., Yamato, M., Yokoyama, M., Sakurai, Y., \u0026amp; Okano, T. (1998). Active platelet movements on hydrophobic/hydrophilic microdomain‐structured surfaces. \u003cem\u003eJournal of Biomedical Materials Research: An Official Journal of The Society for Biomaterials, The Japanese Society for Biomaterials, and the Australian Society for Biomaterials\u003c/em\u003e, \u003cem\u003e42\u003c/em\u003e(1), 148-155. https://pubmed.ncbi.nlm.nih.gov/9740017/ \u003c/li\u003e\n\u003cli\u003eNojiri, C., Okano, T., Koyanagi, H., Nakahama, S., Park, K. D., \u0026amp; Kim, S. W. (1993). In vivo protein adsorption on polymers: Visualization of adsorbed proteins on vascular implants in dogs. \u003cem\u003eJournal of Biomaterials Science, Polymer Edition\u003c/em\u003e, \u003cem\u003e4\u003c/em\u003e(2), 75-88. https://pubmed.ncbi.nlm.nih.gov/1486066/\u003c/li\u003e\n\u003cli\u003eRobert S. (2016). 2016 Guidelines of the American Society of Mammalogists for the use of wild mammals in research and education. \u003cem\u003eJournal of mammalogy,\u003c/em\u003e 97 (3), 663\u0026ndash;688, https://academic.oup.com/jmammal/article/97/3/663/2459909\u003c/li\u003e\n\u003cli\u003eGriffin, J. L., Nicholls, A. W., Daykin, C. A., Heald, S., Keun, H. C., Schuppe-Koistinen, I., Robertson, D. (2007). Standard reporting requirements for biological samples in metabolomics experiments: mammalian/in vivo experiments. \u003cem\u003eMetabolomics\u003c/em\u003e, \u003cem\u003e3\u003c/em\u003e(3), 179-188. https://link.springer.com/article/10.1007/s11306-007-0077-z\u003c/li\u003e\n\u003cli\u003eFares, M. M., \u0026amp; Othman, A. A. (2009). Smart pH-sensitive alternating copolymers of (methylacrylamide-hydroxyethylmethacrylate); kinetic and physical properties. \u003cem\u003eJournal of Macromolecular Science, Part A\u003c/em\u003e, \u003cem\u003e47\u003c/em\u003e(1), 61-70. https://www.tandfonline.com/doi/abs/10.1080/10601320903399750\u003c/li\u003e\n\u003cli\u003eGatti, S., Agostini, A., Ferrari, R., \u0026amp; Moscatelli, D. (2017). Synthesis and nanoprecipitation of HEMA-CLn based polymers for the production of biodegradable nanoparticles. \u003cem\u003ePolymers\u003c/em\u003e, \u003cem\u003e9\u003c/em\u003e(9), 389. https://pubmed.ncbi.nlm.nih.gov/30965689/\u003c/li\u003e\n\u003cli\u003edel \u0026Aacute;ngel-S\u0026aacute;nchez, K., Borbolla-Torres, C. I., Palacios-Pineda, L. M., Ulloa-Castillo, N. A., \u0026amp; El\u0026iacute;as-Z\u0026uacute;\u0026ntilde;iga, A. (2019). Development, fabrication, and characterization of composite polycaprolactone membranes reinforced with TiO2 nanoparticles. \u003cem\u003ePolymers\u003c/em\u003e, \u003cem\u003e11\u003c/em\u003e(12), 1955. https://www.mdpi.com/2073-4360/11/12/1955\u003c/li\u003e\n\u003cli\u003eArefi, M. R., \u0026amp; Rezaei-Zarchi, S. (2012). Synthesis of zinc oxide nanoparticles and their effect on the compressive strength and setting time of self-compacted concrete paste as cementitious composites. \u003cem\u003eInternational journal of molecular sciences\u003c/em\u003e, \u003cem\u003e13\u003c/em\u003e(4), 4340-4350. https://pubmed.ncbi.nlm.nih.gov/22605981/\u003c/li\u003e\n\u003cli\u003eCausa, F., Battista, E., Della Moglie, R., Guarnieri, D., Iannone, M., \u0026amp; Netti, P. A. (2010). Surface investigation on biomimetic materials to control cell adhesion: the case of RGD conjugation on PCL. \u003cem\u003eLangmuir\u003c/em\u003e, \u003cem\u003e26\u003c/em\u003e(12), 9875-9884. https://pubmed.ncbi.nlm.nih.gov/20349926/\u003c/li\u003e\n\u003cli\u003ePrime, K. L., \u0026amp; Whitesides, G. M. (1991). Self-assembled organic monolayers: model systems for studying adsorption of proteins at surfaces. \u003cem\u003eScience\u003c/em\u003e, 1164-1167. https://www.science.org/doi/10.1126/science.252.5009.1164\u003c/li\u003e\n\u003cli\u003eShahverdi, M., Seifi, S., Akbari, A., Mohammadi, K., Shamloo, A., \u0026amp; Movahhedy, M. R. (2022). Melt electrowriting of PLA, PCL, and composite PLA/PCL scaffolds for tissue engineering application. \u003cem\u003eScientific Reports\u003c/em\u003e, \u003cem\u003e12\u003c/em\u003e(1), 19935. https://pubmed.ncbi.nlm.nih.gov/36402790/\u003c/li\u003e\n\u003c/ol\u003e"}],"fulltextSource":"","fullText":"","funders":[],"hasAdminPriorityOnWorkflow":false,"hasManuscriptDocX":true,"hasOptedInToPreprint":true,"hasPassedJournalQc":"","hasAnyPriority":false,"hideJournal":true,"highlight":"","institution":"","isAcceptedByJournal":false,"isAuthorSuppliedPdf":false,"isDeskRejected":"","isHiddenFromSearch":false,"isInQc":false,"isInWorkflow":false,"isPdf":false,"isPdfUpToDate":true,"isWithdrawnOrRetracted":false,"journal":{"display":true,"email":"
[email protected]","identity":"researchsquare","isNatureJournal":false,"hasQc":true,"allowDirectSubmit":true,"externalIdentity":"","sideBox":"","snPcode":"","submissionUrl":"/submission","title":"Research Square","twitterHandle":"researchsquare","acdcEnabled":true,"dfaEnabled":false,"editorialSystem":"","reportingPortfolio":"","inReviewEnabled":false,"inReviewRevisionsEnabled":true},"keywords":"electrospinning, scaffold, wound, Zinc oxide, Titanium oxide","lastPublishedDoi":"10.21203/rs.3.rs-3833998/v1","lastPublishedDoiUrl":"https://doi.org/10.21203/rs.3.rs-3833998/v1","license":{"name":"CC BY 4.0","url":"https://creativecommons.org/licenses/by/4.0/"},"manuscriptAbstract":"\u003cp\u003eThe goal of this experiment is to produce a nanocomposite porous scaffold, using an electrospinning method that has biological properties to use as a skin tissue engineering (TE) and wound dressing. Polyhydroxyethyle methacrylate (PHEMA), polycaprolactone (PCL), Titanium oxide (TiO\u003csub\u003e2\u003c/sub\u003e) nanoparticles, and zinc oxide (ZnO) nanoparticles, used to fabricate this scaffold. After the polymers were synthesized, both polymers were dissolved in chloroform, and nanoparticles were added. The diameter of the fibers obtained depends on the amount of addition of each nanoparticle, the injection rate of the device and the voltage, and the distance between the collector and the needle. Scanning electron microscopy (SEM) images showed the morphology of the scaffold and the cells can adhere well to nanofibers. The mechanical property test showed appropriate mechanical properties for this polymeric scaffold. X-ray diffraction pattern (XRD) and Fourier transform infrared spectroscopy (FTIR) results confirm the successful loading of nanoparticles into the polymer scaffold. Other biological features are characterized with, in vivo assay and MTT and antibacterial assay. The results show that this scaffold is suitable to use as a skin tissue scaffold and wound dress.\u003c/p\u003e","manuscriptTitle":"Development of wound healing scaffold using ZnO and TiO2 nanoparticles","msid":"","msnumber":"","nonDraftVersions":[{"code":1,"date":"2024-01-08 17:28:53","doi":"10.21203/rs.3.rs-3833998/v1","editorialEvents":[{"type":"communityComments","content":0}],"status":"published","journal":{"display":true,"email":"
[email protected]","identity":"researchsquare","isNatureJournal":false,"hasQc":true,"allowDirectSubmit":true,"externalIdentity":"","sideBox":"","snPcode":"","submissionUrl":"/submission","title":"Research Square","twitterHandle":"researchsquare","acdcEnabled":true,"dfaEnabled":false,"editorialSystem":"","reportingPortfolio":"","inReviewEnabled":false,"inReviewRevisionsEnabled":true}}],"origin":"","ownerIdentity":"8f13470b-7813-4b0a-8f04-7a07d29c5dd3","owner":[],"postedDate":"January 8th, 2024","published":true,"recentEditorialEvents":[],"rejectedJournal":[],"revision":"","amendment":"","status":"posted","subjectAreas":[],"tags":[],"updatedAt":"2024-01-25T13:05:38+00:00","versionOfRecord":[],"versionCreatedAt":"2024-01-08 17:28:53","video":"","vorDoi":"","vorDoiUrl":"","workflowStages":[]},"version":"v1","identity":"rs-3833998","journalConfig":"researchsquare"},"__N_SSP":true},"page":"/article/[identity]/[[...version]]","query":{"redirect":"/article/rs-3833998","identity":"rs-3833998","version":["v1"]},"buildId":"qtupq5eGEP_6zYnWcrvyt","isFallback":false,"isExperimentalCompile":false,"dynamicIds":[84888],"gssp":true,"scriptLoader":[]}
Text is read by the "Ask this paper" AI Q&A widget below.
Extraction quality varies by source — PMC NXML preserves structure
cleanly, OA-HTML may include some navigation residue, and OA-PDF can
have broken hyphenation. The publisher copy
(via DOI)
is the canonical version.